pv magazine reported on 9 November that a Tongwei-led team used a low-cost, screen-printed photoresist etch to build a boron selective emitter on TOPCon cells, reaching about 1,600 Ω/sq in the non-contacted region. Average efficiency rose from 25.82% to 25.98%, and an optimized cell was certified by ISFH at 26.03% with a Voc of 746.5 mV. We read the full paper and summarize the process, the key numbers, the instructive failure of the 'locally boron-doped finger' structure, and the questions that remain before mass production.
On 9 November, pv magazine reported a new TOPCon result from a Tongwei-led team, published in Solar Energy Materials and Solar Cells. In one sentence: without laser patterning, using a low-cost screen-printed photoresist as the mask, the team raised the sheet resistance of the non-contacted front boron emitter to about 1,600 Ω/sq, and an optimized cell was certified by ISFH in Germany at 26.03%. We read the full paper; here are the main points.
01 What the news says
According to pv magazine, the work was led by Tongwei, with partners including the School of Optoelectronic Science and Engineering at the University of Electronic Science and Technology of China (UESTC) and an equipment company, Jiangsu Inspiray Equipment. The subject is the front boron emitter of n-type TOPCon cells, and the approach is a selective emitter (SE): heavy doping under the fingers for contact, light doping between the fingers for lower recombination.
- Sheet resistance pair: about 450 Ω/sq in the contacted P++ region and about 1,600 Ω/sq in the non-contacted P+ region; the reference is a uniform emitter at about 490 Ω/sq. A higher sheet resistance means lighter doping.
- Average efficiency: up from 25.82% to 25.98%, a 0.16% absolute gain; Voc from 742.6 mV to 745.5 mV, FF from 83.54% to 83.76%. Thirty cells per group, from the same production batch.
- Certified efficiency: 26.03% for an optimized cell, certified by ISFH, with a Voc of 746.5 mV.
- The other structure: a 'locally boron-doped finger' design with a fully undoped non-contacted region gained only about 0.04%; the problem was FF.
02 Why the non-contacted sheet resistance matters
A uniform emitter has a long-standing conflict. Heavy doping gives good metal contact but high surface and Auger recombination, so the emitter saturation current density J0e (a measure of emitter recombination; lower is better) is high. Light doping does the opposite: passivation improves, but contact resistance and lateral transport resistance go up.
In recent years, laser-assisted firing (LECO/LIF) has made good contacts possible on lightly doped emitters, pushing front sheet resistance above 400 Ω/sq. One study cited in the paper combined a high-sheet-resistance boron emitter with grid optimization to reach a certified 26.66% and a Voc of 744.6 mV. But the paper points out that even with such a uniform high-sheet-resistance emitter, the non-contacted region is still limited by boron-related surface and Auger recombination.
An SE is the natural next step. Yet in the boron SE studies reviewed in the paper, the non-contacted sheet resistance stayed below 300 Ω/sq, and laser SE routes also suffer from thermal damage and an insufficient boron dose in the BSG (borosilicate glass) layer.
| Study (cited in the paper) | SE method | P++/P+ sheet resistance (Ω/sq) | Efficiency gain (abs.) |
|---|---|---|---|
| Lin et al., 2020 | Green laser doping | 54 / 95 | 0.24% |
| Wang et al., 2023 | 3D-printed mask + second boron diffusion | ~75 / 230 | 0.27% |
| Li et al., 2023 | Mask + etch-back | P+ 230-280 | 0.34% |
| This work | Screen-printed photoresist etch | ~450 / 1,600 | 0.16% |
Note that each study used a different baseline, so the gains cannot be ranked directly. The baseline here is already a 490 Ω/sq high-sheet-resistance emitter with LIF at 25.82%, so the 0.16% comes on top of a fairly high starting point.
03 The process: screen-printed photoresist as the mask
The paper calls the flow PR etch. The idea: do a first boron diffusion, cover the future contact regions with photoresist, etch away everything else together with the existing p-n junction, then dope lightly a second time.

Fig. 1 Main steps of the PR-etch selective emitter process (redrawn from the paper's description)
A few details are worth noting. The photoresist resists HF and dissolves in dilute alkaline solution. The paper gives a price of about USD 14/kg, or roughly USD 0.0015 per wafer in material cost. The second texturing etches about 3 μm deep. During the second high-temperature oxidation (1,040°C, 80 min), boron at the surface of the P++ region segregates into the BSG layer, lowering the surface concentration and deepening the junction, so the sheet resistance goes from about 350 Ω/sq after the first diffusion to about 450 Ω/sq.
The paper also states explicitly that 'laser-free' refers only to the SE patterning step. After firing (peak 875°C), the cells still received light injection and laser-induced firing (LIF) to improve the contact between silver and the boron emitter.
04 Key data: J0e from 7.2 down to about 4 fA/cm²
Passivation first. QSSPC measurements on double-sided symmetric samples give a single-side J0e of about 7.2 fA/cm² for the baseline emitter (490 Ω/sq), about 4.5 fA/cm² at a P+ sheet resistance of 800 Ω/sq, and a slow further decline to around or below 4 fA/cm² at 1,200-2,000 Ω/sq.

Fig. 2 Emitter J0e versus sheet resistance, and the recombination breakdown from the EDNA 2 model
The paper breaks this down with the EDNA 2 model: going from 490 to 1,600 Ω/sq, the surface-related component falls from 6.51 to 3.84 fA/cm², and the Auger component from 0.68 to 0.17 fA/cm². In other words, most of the benefit comes from lower surface recombination.
The symmetric samples actually reached about 2,000 Ω/sq, but 1,600 Ω/sq was chosen for full cells, for two reasons: beyond 1,600 Ω/sq the further drop in J0e is small, while within-wafer sheet resistance non-uniformity tends to get worse.

Fig. 3 Mean electrical parameters of the three front structures (30 cells per group)
At cell level, the SE gain comes mainly from Voc (+2.9 mV) and FF (+0.22%), with Jsc comparable to the baseline. Series resistance Rs rises slightly, which the paper attributes to higher lateral transport resistance in the high-sheet-resistance non-contacted region. The certified cell area is 389.3 cm² (read from the certified I-V figure in the paper).
Takeaway: Raising the non-contacted sheet resistance from 490 to 1,600 Ω/sq cuts J0e from about 7.2 to about 4 fA/cm²; average cell efficiency rises by 0.16% absolute, with 26.03% certified. Going higher brings less passivation gain and worse uniformity.
05 A useful negative result: leaving the non-contacted region undoped
If lighter doping passivates better, why not leave the non-contacted region undoped altogether? The paper tested this as the 'locally boron-doped finger' structure: after the second texturing, no boron is deposited, only the high-temperature oxidation is applied.
Voc did go up (745.1 mV), but FF was only 83.34%, 0.42% below the SE structure, leaving the efficiency just about 0.04% above baseline. Rs was only about 0.01 Ω·cm² higher than in the SE group; using the empirical relation cited in the paper, ΔFF ≈ Rs × 5%, that explains only about 0.05% of the FF gap.

Fig. 4 FF loss of the locally boron-doped finger structure: series resistance explains only a small part
For the rest, the paper points to junction-edge recombination. The second texturing etches about 3 μm deep, far more than the P++ junction depth, so the step sidewall cuts through the original boron-diffused layer and exposes a p-n junction edge and an undoped sidewall. With 276 fingers and two sidewalls each, that is about 552 longitudinal junction edges. In the SE structure, the second boron diffusion also forms a P+ layer on the sidewall, keeping the front junction laterally continuous; cross-sectional EBIC (electron-beam-induced current) images support this.
The PL (photoluminescence) results fit as well: at 1 sun, the finger group shows higher PL intensity than the baseline; at 0.1 sun it falls below the baseline, indicating greater sensitivity to low-injection recombination, the kind of junction-edge loss that mainly reduces FF. The paper is candid, however, that the available characterization supports this explanation only qualitatively and cannot quantify it.
06 Where the simulations point
The paper ran Quokka3 device simulations. The following are simulated trends that still need experimental validation:
- Contacted-region width: within the range examined, efficiency peaks at a P++ width of about 200 μm; wider than that, recombination in the heavily doped area offsets the passivation gain.
- Finger width and pitch: with fingers narrowed to 7-9 μm, the optimal pitch shifts to about 500-550 μm and efficiency can rise further. A high-sheet-resistance SE has to be optimized together with finer, denser fingers.
- Wafer resistivity: efficiency rises with bulk resistivity for both structures. The simulations suggest the finger structure could benefit more from high-resistivity wafers, but they do not include junction-edge recombination, and the paper says explicitly that this part should not be read quantitatively.
07 Our view
We see three points of value. First, it offers a process route that does not rely on laser patterning and takes the non-contacted sheet resistance above 1,000 Ω/sq, backed by a third-party certified efficiency. Second, it answers 'how high is high enough': around 1,600 Ω/sq is the compromise between passivation gain and uniformity. Third, it reports honestly why the finger structure fell short, which is a useful reference for teams considering a 'local emitter' route.
The limitations matter too. Compared with a uniform-emitter flow, PR etch adds printing, UV curing, BSG etching, resist stripping, a second texturing and a second boron diffusion (including oxidation at 1,040°C for 80 min). The USD 0.0015 per wafer covers photoresist material only; the main text does not work through equipment, energy, throughput or yield. The data come from one batch with 30 cells per group; the alignment window between printed fingers and contact regions about 200 μm wide, and sheet resistance uniformity at volume, will need production data.
From a module and reliability standpoint, we would add one more question: the main text gives no stability data for the super-high-sheet-resistance emitter under UV, damp heat or similar stress, and no module-level results.
Bottom line: A front-side TOPCon efficiency idea backed by certified data and a credible process; cost, alignment, uniformity and reliability still stand between it and mass production.
08 Final thoughts
While BC and tandems dominate the conversation, this paper is a reminder that the TOPCon front emitter still has room to give, and the direction is clear: lighter doping between the contacts, narrower contact regions, finer and denser fingers. Whether that is achieved with photoresist, lasers or something else will be decided by cost and yield on the production line.
Calculation notes / data basis
- The certified cell's area (389.3±1.6 cm²), Isc (16,178±180 mA), FF (83.89±0.92%) and Pmpp (10,132±150 mW) are read from the labels in Fig. 4(f) of the paper; the main text gives only 26.03% and 746.5 mV. Our check, Pmpp ÷ area, gives about 26.03%, in line with the certified value.
- The 25.86% average efficiency of the locally boron-doped finger structure, the mean Jsc of the three groups (baseline 41.62, SE 41.60, finger 41.65 mA/cm²) and the mean Rs (0.560/0.571/0.583 Ω·cm²) are read from the labels in Fig. 4 of the paper; the main text states 'a gain of about 0.04%'. Our Voc × Jsc × FF check of the three groups (25.82%/25.98%/25.86%) matches the figure labels.
- The totals on the right of Fig. 2 are our own sums: 6.51 + 0.68 = 7.19 fA/cm² at 490 Ω/sq and 3.84 + 0.17 = 4.01 fA/cm² at 1,600 Ω/sq, consistent with the measured ~7.2 and ~4 fA/cm². The left panel plots only the two points for which the main text gives values; for 1,200-2,000 Ω/sq the text says only 'around or below 4 fA/cm²', shown as a band.
- The 'about 0.37% beyond series resistance' in Fig. 4 is our own subtraction (0.42% − 0.05%); the paper does not attribute this part quantitatively.
- USD 0.0015 per wafer is photoresist material cost only (as stated in the paper), excluding equipment and energy for printing, curing, wet processing and the second diffusion.
- Partner institutions follow the pv magazine report. The paper's supplementary material was not obtained; statements on uniformity and cost details follow the main text only.
- The journal page lists an issue date of 15 January 2027; the online publication date was not verified. No ISFH certificate number appears in the main text.
References
- Liu Q., Yu B., He Y., et al. High-efficiency TOPCon solar cells featuring super-high sheet resistance emitters via low-cost photoresist etching. Solar Energy Materials and Solar Cells, 2027, 114810. https://doi.org/10.1016/j.solmat.2026.114810
- Bellini E. Tongwei unveils 26.03%-efficient TOPCon solar cell with high sheet resistance. pv magazine Global, 2026-11-09. https://www.pv-magazine.com/2026/11/09/tongwei-unveils-26-0-3-efficient-topcon-solar-cell-with-high-sheet-resistance/
- Yang Z., Chen S., Mao J., et al. Dual-side electrical refinement enables efficient industrial tunnel oxide passivating contact silicon solar cells. Nature Energy, 2026. https://doi.org/10.1038/s41560-026-01982-2
PV Materials Lab
https://pvmaterialslab.com
PV Materials Lab
A PV R&D and technical team with 10+ years of experience | In-depth technical knowledge sharing
Materials · Reliability · Failure Analysis · Standards & Certification · Products · Processes
Exploring AI + PV — collaboration welcome
Disclaimer:
- Original content reflects the authors' personal views only, is for reference, and does not constitute investment advice.
- Reposted and cited content is credited to its source, with respect for original work.
- Some content is AI-assisted (chart generation, data retrieval, concept explanations, etc.); the core framework and key content are written by our technical team and reviewed by humans.
- For any inaccuracy or infringement, please leave a message or contact us.