Skip to content

Hail, Breakage, PID: The Role of Glass in Module Reliability ​

Cover

In brief

Glass stands behind many module reliability problems: hail smashing the front sheet, glass-glass modules breaking "for no reason", sodium migration triggering PID, coating degradation dragging down yield... This article groups glass-related reliability risks into four categories, mechanical, optical, electrical and encapsulation, and, drawing on IEC standards and recent work by NREL, CEA and Kiwa PVEL, explains the mechanism of each risk, the role glass plays and what can be done at module level.

In the previous article we covered the "health check" of PV glass. But glass that passes does not guarantee a reliable module. As glass goes into a module, the module onto a racking system and the racking out into the field, each layer adds new stresses. The hottest industry topics of the past two years, hail losses and glass-glass breakage, both centre on glass. In this article we look at the glass again from the perspective of module reliability.

We group module reliability risks directly related to glass into four categories: mechanical, optical, electrical and encapsulation. Mechanical risks attract the most attention and are the category in which failures have grown fastest in recent years.

Figure 1. Module reliability risks related to PV glass

Figure 1. Module reliability risks related to PV glass

Kiwa PVEL's module reliability scorecard published in May 2026 showed that a record 87% of participating manufacturers had at least one test failure (up from 66% two years earlier), 61% of bills of materials (BOMs) had at least one failure, and about 30% of BOMs failed in the mechanical stress sequence (MSS). The organisation stated bluntly that failure rates for delamination and mechanical breakage have reached new highs. Glass is unavoidably at the centre of these figures.

02Hail: the most direct test a module faces ​

Hail is the most direct test of front glass. The standard hail test in IEC 61215 fires 25 mm ice balls at 23 m/s at specified points on the module. But real hail can be far larger. We worked out the kinetic energy from the mass and speed of the ice balls:

Figure 2. Impact energy of hail of different diameters versus glass ball-drop thresholds (estimate)

Figure 2. Impact energy of hail of different diameters versus glass ball-drop thresholds (estimate)

A 25 mm hailstone carries less than 2 J, a 45 mm one about 20 J, and a 75 mm one more than 150 J. Doubling the hail diameter raises the energy by nearly an order of magnitude. Compared with the ball-drop thresholds in article 06, about 2.2 J for 2.0 mm glass and about 10.2 J for 3.2 mm, it is easy to see why modules that pass the standard test can still break en masse in large hail. Kiwa PVEL's 45 mm hail testing bears this out: glass-glass modules with 2 mm glass on both sides accounted for 61% of the hail breakages, while modules with 3.2 mm front glass accounted for only 7%.

The losses are real. According to a 2026 review involving the European Severe Storms Laboratory (ESSL), Europe recorded 9,882 large-hail events in 2023, and hail damage in northern Italy in July of that year was about EUR 6 billion. In 2019, hail struck a utility-scale plant in Texas, and 400,000 of its 650,000 modules had to be replaced.

On the glass side, the main defence against hail is greater thickness and strength, for example choosing thicker front glass in hail-prone regions. On the system side, trackers can move to a protective stow angle before hail arrives, and protective nets can be installed. Hail test frameworks stricter than IEC 61215 also exist, such as IEC TS 63397, for assessing modules in high hail-risk regions.

Summary

The standard hail test is a "pass mark", not a "safety line". In high hail-risk regions, glass thickness and strength should be chosen for the local hail size, not for the standard.

03Breakage "for no reason": a new problem of the glass-glass era ​

Even more troublesome for the industry than hail is "spontaneous" breakage with no obvious external impact. Research by the US National Renewable Energy Laboratory (NREL) at the end of 2024 found that such breakage is more common in modules with glass thinner than 3.2 mm, and especially concentrated in glass-glass modules with glass around 2 mm.

There is no single cause. Both NREL and the consultancy CEA point out that it results from several factors combined:

Figure 3. Multiple causes of glass breakage in the field

Figure 3. Multiple causes of glass breakage in the field

  • The glass itself: 2.0 mm heat-strengthened glass has lower surface compression than 3.2 mm fully tempered glass to begin with, leaving less strength margin; surface stress varies between glass sources, and some glass measures close to the lower thickness limit, within spec but with little margin; poor edge finishing, internal bubbles and inclusions become stress concentrators.
  • Module design: formats keep growing, so deflection under the same wind and snow loads increases; some modules leave the factory with pre-stress from lamination or framing. The frame matters too: Kiwa PVEL found that about 62% of MSS failures were related to frame stiffness, and breakage rates doubled when frame height fell below 35 mm.
  • Installation and racking: cracks often start near clamps, at corners and where the frame carries load; poor clamp position and torque, tracker torsion and continuous vibration all amplify fatigue damage.
  • The gap between standards and reality: clamp positions in lab tests often differ from those in the field, and torsional loads are not part of routine testing, so modules can pass IEC 61215 certification and still break in the field.

It is worth noting that NREL also called the idea that "2 mm glass cannot be fully tempered" a common misconception: it can be done with the right equipment. This does not contradict article 05: being able to do it and doing it economically at scale are two different things; the bottlenecks for tempering thin glass are cost, flatness and yield.

On breakage, CEA's recommendations, as reported by pv magazine, include testing with the project's actual mounting method and including dynamic loads, matching clamp design and spacing to the glass and frame characteristics, batch traceability for glass, and systematic checks of edge quality, inclusions and lamination stress.

04PID: the sodium in the glass ​

We covered PID (potential-induced degradation) in our PID series; here we focus only on the role of glass.

Figure 4. Sodium migration from glass causing PID (schematic)

Figure 4. Sodium migration from glass causing PID (schematic)

PV glass is a soda-lime-silica glass containing about 13% sodium oxide. When there is a high voltage between the cells and the grounded frame, combined with high temperature and humidity, sodium ions in the glass are driven by the electric field through the encapsulant towards the cell surface, damaging the cell's surface passivation and field and causing leakage and power loss. A water film forming on the glass surface in damp conditions provides a path for leakage current.

PID is countered mainly through encapsulant barrier properties, optimised cell surface layers and system grounding, with glass playing a relatively passive role. But it is a reminder that glass is not an "inert" sheet; it takes part in the chemical and electrical processes inside a module.

05Optics and encapsulation: sources of slow degradation ​

Unlike breakage, the following problems do not scrap a module on the spot, but over years or a decade or more they slowly eat into energy yield:

RiskSymptomLink to glassMitigation
AR coating degradationTransmittance falls year by yearPorous coatings wear easily under sand and cleaning brushesChoose durable coatings; standardise cleaning
Surface corrosion / mouldWhite spots, haze on the glassMoisture in storage and transport; sodium leaches and attacks the surfaceControl storage humidity; standardise packaging
SoilingDirt shading the surfaceCoating surface properties affect soiling and cleaningRegular cleaning; some coatings are easy-clean
Moisture ingressInternal corrosion, delaminationGlass is nearly impermeable; edges are the main pathEdge sealing and encapsulant choice
Acetic acid build-up in glass-glassCorrosion of ribbons and fingersGlass-glass does not breathe, so acetic acid from EVA cannot escapeGlass-glass mostly uses POE or EPE encapsulants

Table 1. Slow-degradation risks related to glass

The last item shows how one material choice ripples through the others: a glass-glass build is a good barrier that keeps external moisture out, but it also keeps acetic acid generated inside from escaping. The choice of glass design in turn changes the choice of encapsulant, one reason glass-glass modules are commonly paired with POE-type encapsulants.

06Final thoughts ​

Returning to the four roles set out in article 01, this article has really looked at what happens when each role "fails": when the structural backbone fails, we get hail damage and breakage; when the optical window fails, coating degradation and corrosion; and when the protective barrier and insulation roles fail, moisture, acetic acid and PID.

The more important conclusion is that glass reliability is never about the glass alone. It is tightly bound up with module format, frame, encapsulant, mounting method and local climate. Looking only at the glass specification will never show the whole risk picture.

Bottom line

Glass that passes is only the starting point; module reliability depends on a matched system of glass, module design, installation and environment.

In the next article we go to the failure scene: spontaneous breakage, thermal stress cracking, installation damage, whitened coatings, mouldy glass... What are the common failures of PV glass, and how can the fracture pattern reveal the cause? Stay tuned. We would be glad to hear from you.

Calculation notes / data basis: 1. Hail kinetic energy is estimated as E = ½mv², with ice density 0.9 g/cm³ and speeds for each diameter taken from the IEC 61215 hail test parameter table (e.g. 25 mm: m ≈ 7.4 g, v = 23.0 m/s, E ≈ 1.9 J; 75 mm: m ≈ 199 g, v = 39.5 m/s, E ≈ 155 J); ball-drop thresholds are E = mgh (h = 1 m). The impact modes differ, so this is an order-of-magnitude comparison only. 2. Kiwa PVEL 2026 scorecard data are from PV Tech and TaiyangNews reports; European hail event and loss data and the Texas plant data are from pv magazine's report on a review published in Energy Reports. 3. Sodium oxide content of about 13% is a typical value for soda-lime-silica PV glass; see article 03 of this series.

References

  1. PV Tech: Module test failures continue to increase in Kiwa PVEL's 2026 Module Reliability Scorecard, 2026-05, https://www.pv-tech.org/module-test-failures-continue-to-increase-in-kiwa-pvels-2026-module-reliability-scorecard/
  2. TaiyangNews: PV Module Failures Increase Under Mechanical And Environmental Stress Tests, 2026, https://taiyangnews.info/technology/kiwa-pvel-2026-module-reliability-testing-scorecard
  3. pv magazine: Kiwa PVEL's 2026 solar module reliability scorecard reveals high failure rates, 2026-05-28
  4. pv magazine: When hail hits PV: New research maps damage, testing, and mitigation, 2026-02-24, https://www.pv-magazine.com/2026/02/24/when-hail-hits-pv-new-research-maps-damage-testing-and-mitigation/
  5. pv magazine: CEA recommendations for mitigating glass breakage, 2025-07-28, https://www.pv-magazine.com/2025/07/28/cea-recommendations-for-mitigating-glass-breakage/
  6. PV Tech: NREL says thinner, taller solar modules contributing to increased rate of breakages, 2024-12-11, https://pv-tech.org/nrel-finds-thinner-taller-modules-contributing-increased-rate-breakages
  7. IEC 61215-2:2021, Terrestrial photovoltaic (PV) modules — Design qualification and type approval — Part 2: Test procedures
  8. China Photovoltaic Industry Association: T/CPIA 0028.1—2024 Glass for photovoltaic modules — Part 1: Front plate anti-reflective coated glass, 2024
PV Materials Lab
https://pvmaterialslab.com
PV Materials Lab
A PV R&D and technical team with 10+ years of experience | In-depth technical knowledge sharing
Materials · Reliability · Failure Analysis · Standards & Certification · Products · Processes
Exploring AI + PV — collaboration welcome

Disclaimer:
1. Original content reflects the authors' personal views only, is for reference, and does not constitute investment advice.
2. Reposted and cited content is credited to its source, with respect for original work.
3. Some content is AI-assisted (chart generation, data retrieval, concept explanations, etc.); the core framework and key content are written by our technical team and reviewed by humans.
4. For any inaccuracy or infringement, please leave a message or contact us.