What Tests Must PV Glass Pass? Key Indicators and Test Methods Explained

In brief
Between leaving the factory and going into a module, a sheet of PV glass goes through more than twenty tests in four groups: optical, dimensions and appearance, mechanical, and coating and durability. Using T/CPIA 0028.1—2024 as the main thread, this article explains, item by item, what transmittance, surface stress, ball-drop impact, four-point bending, fragmentation and the ageing tests check, how they are measured and where the thresholds lie, and discusses several points that incoming inspection should watch beyond the standard.
The previous five articles covered what PV glass does, how it is classified, its raw materials and its processes. Once the glass is made, how do we judge whether it is up to standard? In this article we open the "health check" of PV glass and look at the hurdles it has to clear. The indicators and methods here are based mainly on the China Photovoltaic Industry Association standard T/CPIA 0028.1—2024, "Glass for photovoltaic modules — Part 1: Front plate anti-reflective coated glass".
01The big picture: four groups, more than twenty tests
Mapping the "four roles" from article 01 onto testing, PV glass tests fall roughly into four groups: optical performance, dimensions and appearance, mechanical performance, and coating and durability.

Figure 1. Main tests for front PV glass
These tests are of two kinds. Routine (release) tests are carried out on every batch, mainly dimensions, appearance, bow, colour uniformity and transmittance; they are fast and non-destructive and can be done inline or by sampling. Type tests are carried out when a new product is finalised or moved to a new plant, when structure, materials or process change significantly, when production resumes after a long stop, or when routine results differ markedly from the last type test, and at least once a year in normal production. They include the mechanical and durability tests, take a long time and are mostly destructive.
Routine tests check whether "this batch has a problem"; type tests check whether "this product design and process can be trusted". Both are indispensable.
02Optical performance: transmittance and iron content
PV transmittance is the most important indicator for PV glass. Unlike ordinary "visible transmittance", it covers the 380–1100 nm band, matching the response range of crystalline silicon cells. Three samples of at least 300 × 300 mm are measured at five specified areas each with a spectrophotometer, and the results are averaged. The standard requires at least 93.8% for a single-layer coating and at least 94.1% for a double-layer coating.
Iron content is determined by the chemical analysis method for soda-lime-silica glass, with Fe₂O₃ required to be no more than 0.015%. It is not a routine test, but it is the "source indicator" for transmittance. As explained in article 03, the oxidation state of iron also affects transmittance, so passing on iron content does not guarantee passing on transmittance; the two must be looked at together.
Colour uniformity is checked visually in a specified light box, with no obvious colour difference allowed. It looks like a cosmetic issue, but it usually reflects how uniform the coating thickness is.
03Dimensions and appearance: quality you can see
For dimensions, 2.0 mm-class glass has a thickness tolerance of ±0.15 mm, and the difference between the mid-points of the four edges of one sheet must not exceed 0.25 mm. For bow, overall bow must not exceed 0.2%; for 1.6–2.5 mm glass, roller wave must not exceed 0.4 mm over any 300 mm, and edge lift within 25 mm of the edge must not exceed 0.5 mm.
The impact of flatness at module level is often underestimated. Uneven glass leads to uneven local pressure during lamination, easily causing bubbles and cell microcracks, and glass-glass modules are especially sensitive.
Appearance is inspected in an environment free from outside light: the sample stands vertically in front of a matt black screen under fluorescent lighting of about 700 lx, with the observer 600 mm away. The standard limits the number of defects such as bubbles, stones, scratches and edge chips by size class, while roll marks, iridescence, mould, cracks, open bubbles and black inclusions are not allowed at all.
04Mechanical performance: surface stress is the "master switch"
Mechanical tests check the "structural backbone" role. The most critical and most widely used is surface stress, because it directly shows whether tempering has been done properly, and it can be measured non-destructively.
Surface stress is measured with a surface stress meter based on photoelasticity, on the patterned, uncoated side at nine points: four corner points more than 100 mm from the edge and one centre point, plus four edge points no more than 100 mm from the edge, distinguishing the end that leaves the furnace first from the end that leaves last. Three numbers are reported: the minimum as the single-point value, the arithmetic mean as the average, and the difference between maximum and minimum as the range.

Figure 2. Nine measuring points for surface stress (schematic)
| Thickness | Single-point value | Mean | Range |
|---|---|---|---|
| 3.2 mm | ≥90 MPa | ≥95 MPa | <15 MPa |
| 2.0 mm | ≥60 MPa | ≥65 MPa | <15 MPa |
Table 1. Surface stress requirements (T/CPIA 0028.1—2024)
The range deserves special attention. If the mean passes but the range is large, tempering is uneven and the glass has "weak spots", and breakage tends to start at the weakest place. So never read only the mean on a report.
The other mechanical tests verify strength from different angles:
- Ball-drop impact: a steel ball is dropped from 1 m onto the centre of the glass; the sample passes if it does not break. Ball mass depends on thickness: 227 g for 2.0 mm and below, 535 g for 2.0–2.8 mm, and 1040 g above 2.8 mm.
- Four-point bending strength: two support rollers hold the glass while two loading rollers press down from above at a constant rate until it breaks; the result is valid only if the fracture origin lies between the two loading rollers. The mean must be at least 140 MPa for 2.0 mm and 145 MPa for 3.2 mm.
- Fragmentation: for fully tempered glass only, the fragments within a 50 × 50 mm area are counted after breakage: at least 15 for 2.5 mm and below, and at least 40 above 2.5 mm. There is no requirement for heat-strengthened glass.
- Shot-bag impact: following the method in the architectural tempered glass standard GB 15763.2, a pendulum shot bag filled with lead shot strikes the glass to check safety under large-area impact; all four samples must pass.
- Thermal shock: a hot-air gun heats a local area of the glass to 200 °C within 30 seconds, at the centre, the edge mid-points and the corners, to check resistance to local temperature differences, corresponding to scenarios such as hot spots in modules.

Figure 3. Steel ball mass and impact energy in the ball-drop test
Converting ball mass into impact energy makes it intuitive: 2.0 mm glass must withstand about 2.2 J, 3.2 mm about 10.2 J, a difference of nearly five times. Thin glass has a far lower impact threshold to begin with, the price that has to be paid for going thinner.

Figure 4. Four-point bending test (schematic)
05Coating and durability: the "longest" part of the standard
The durability of the AR coating underpins long-term energy yield. The standard sets out a full series of tests with a single pass criterion: after each test, transmittance loss must not exceed 1%, and the coating must show no obvious peeling, delamination or wrinkling.
| Test | Main conditions | Scenario simulated |
|---|---|---|
| Pencil hardness | Coating at least 3H | Everyday scuffs |
| Washing | 400 back-and-forth strokes | Plant cleaning |
| Acid resistance | 1 mol/L hydrochloric acid, 23 °C, 24 h immersion | Acid rain, pollution |
| Neutral salt mist | 96 h | Coastal environments |
| Thermal cycling | −40 °C to 85 °C, 200 cycles | Day–night and seasonal swings |
| Humidity freeze | 10 cycles | Freezing after high humidity |
| Damp heat | 85 °C / 85% RH, 1000 h | Hot, humid climates |
| UV | 15 kWh/m² at 280–385 nm, sample at about 60 °C | Long-term sun exposure |
| Sand and dust | Blowing dust, blowing sand (18–29 m/s, 90 min), settling dust | Deserts and gravel plains |
| PCT | 121 °C, saturated humidity, 48 h | Accelerated damp-heat ageing |
Table 2. Coating durability test conditions (T/CPIA 0028.1—2024)
Many of these test conditions are borrowed directly from the module-level IEC 61215. At module level, glass also has to pass, together with the other materials, tests such as static load and hail (25 mm ice balls at 23 m/s).
06Beyond the standard: what incoming inspection should watch
The standard is a threshold, not the whole picture. Based on module-side experience, we think several points deserve extra attention in incoming inspection:
- Look at the distribution, not just the mean: for both transmittance and surface stress, look at point-to-point distribution and batch-to-batch variation, especially the surface stress range and the edge-point values.
- Keep an eye on edge quality: edge finishing, chips and hole-edge treatment are only constrained by appearance rules in the standard, yet they are closely linked to field breakage of modules.
- Watch how flatness affects lamination: glass that passes on bow can still cause problems when laminating large glass-glass modules, so assess it together with lamination yield.
- Look at trends in durability tests: the 1% loss threshold is a "pass mark"; two coatings that both pass, one losing 0.2% and the other 0.9%, may perform very differently over the long term.
07Final thoughts
The health check of a sheet of PV glass essentially verifies whether it can fulfil the four roles described in article 01: transmittance and iron content for the optical window; surface stress, ball drop and bending strength for the structural backbone; and the durability tests for long-term protection.
Understanding this health check means understanding glass suppliers' specifications and test reports; understanding the limits of the standard tells you which risks you need to check again yourself at incoming inspection and at module level.
The standard tells us whether glass "passes"; distribution, edges and trends tell us whether it can be "trusted".
In the next article we move from the glass itself to the module: what role does glass play in module reliability? Which risks, such as hail, mechanical load, PID and coating degradation, are directly related to glass? Stay tuned. We would be glad to hear from you.
References
- China Photovoltaic Industry Association: T/CPIA 0028.1—2024 Glass for photovoltaic modules — Part 1: Front plate anti-reflective coated glass, https://www.ttbz.org.cn/Home/PdfFileStreamGet/c3QsMTM5NzQ4
- China Photovoltaic Industry Association: T/CPIA 0028.2—2024 Glass for photovoltaic modules — Part 2: Reflective-coated rear glass for glass-glass modules, https://www.ttbz.org.cn/Home/PdfFileStreamGet/c3QsMTM5NzQ3
- GB/T 30984.1—2015 Solar glass — Part 1: Ultra-clear patterned glass
- GB 15763.2—2005 Safety glazing materials in building — Part 2: Tempered glass
- IEC 61215-2:2021, Terrestrial photovoltaic (PV) modules — Design qualification and type approval — Part 2: Test procedures
https://pvmaterialslab.com
A PV R&D and technical team with 10+ years of experience | In-depth technical knowledge sharing
Materials · Reliability · Failure Analysis · Standards & Certification · Products · Processes
Exploring AI + PV — collaboration welcome
Disclaimer:
1. Original content reflects the authors' personal views only, is for reference, and does not constitute investment advice.
2. Reposted and cited content is credited to its source, with respect for original work.
3. Some content is AI-assisted (chart generation, data retrieval, concept explanations, etc.); the core framework and key content are written by our technical team and reviewed by humans.
4. For any inaccuracy or infringement, please leave a message or contact us.