Reading What Fragments Say: Common PV Glass Failures and How to Analyse Them ​

Cover

In brief

When PV glass breaks, was it spontaneous breakage, hail, thermal stress or an installation problem? Every kind of failure leaves a "signature" in the fragments. This article reviews the common failure types of PV glass, shows how to read four typical fracture patterns and how to "find the origin", the first step in failure analysis, and explains the causes and diagnosis of optical failures such as whitened coatings, glass weathering and quench marks.

In the previous article we looked at the four categories of risk glass faces from the perspective of module reliability. This article takes us to the failure scene: when the glass of a module really has broken, turned white or developed patterns, how do we determine the cause? The good news is that glass is an "honest" material: how it broke is mostly written in the fragments.

01An overview of common PV glass failures ​

PV glass failures fall broadly into two groups: breakage, which directly damages the module and may create safety risks; and optical/surface failures, which do not scrap the module immediately but keep dragging down energy yield or cause cosmetic complaints.

GroupFailure typeCommon causes
BreakageSpontaneous breakagePhase-change expansion of nickel sulphide and other inclusions
BreakageImpact breakageHail, flying stones, knocks during installation and O&M
BreakageThermal stress crackingTemperature difference between a hot local area and cooler edges
BreakageLoad / installation crackingWind and snow loads, poor clamping, racking torsion
BreakageTransport and handling damageImpacts at corners and edges
Optical / surfaceWhitened or peeling coatingPoor coating durability; cleaning agents or environmental attack
Optical / surfaceGlass weathering, white stainsMoisture in storage; alkaline attack on the surface
Optical / surfaceQuench marks, iridescenceUneven quenching or uneven coating thickness

Table 1. Common failure types of PV glass

Summary

For breakage, the key is to "find the origin and read the pattern"; for optical failures, the key is to "tell whether the problem lies in the coating or in the glass itself".

02Reading four typical fracture patterns ​

Breakage from different causes produces very different fragment patterns. The figure below shows the four most common:

Figure 1. Four typical fracture patterns (schematic)

Figure 1. Four typical fracture patterns (schematic)

  • Spontaneous breakage: if tiny inclusions such as nickel sulphide (NiS) end up in tempered glass, they slowly transform in service from the high-temperature alpha phase to the stable beta phase, expanding in volume by about 2.5–4%. If an inclusion happens to sit in the tensile zone of the core, it can cause breakage without any external force. The typical signature is an origin inside the glass, with two symmetrical "half-moon" fragments at the origin shaped like a butterfly, a tiny particle at the centre and no impact marks. Spontaneous breakage occurs mainly in fully tempered glass; heat-strengthened glass cools more slowly, giving NiS time to complete its phase change during production, and its core tension is low, so the probability is very small. The architectural glass industry's usual remedy is the "heat soak test": glass is held at about 260–290 °C so that panes at risk break in the oven beforehand.
  • Impact breakage: radial and concentric cracks form around the impact point, which often shows a conchoidal chip on the surface. Hail, flying stones and knocks from tools or hard objects during O&M all produce this pattern, and hail breakage often appears in clusters in the same area.
  • Thermal stress cracking: when part of the glass is heated and expands while the edges, shaded by the frame or cooling fast, stay cooler, tensile stress builds at the edge. Thermal cracks usually start at the edge at right angles to it and meander with few branches, because little energy is released. Hot spots and partial shading can trigger them, which is why the standard includes a thermal shock test.
  • Load / installation cracking: the origin usually lies near a clamp, at a corner or at a support point, and the crack runs roughly perpendicular to the main tensile stress there. If breakage origins across a plant cluster in the same position, for example all at the clamp on one side, an installation or racking problem can essentially be pinpointed.

Another easily overlooked type is transport and handling damage: the origin is usually at a chip on a corner or edge, often a microcrack formed during unpacking, handling or installation that only grows once loaded in the field.

03Finding the origin: the first step in failure analysis ​

The first step in determining a failure's cause is not guessing but finding the crack origin. Where the origin is and what it looks like largely determine the failure type.

Figure 2. Crack branching and locating the origin (schematic)

Figure 2. Crack branching and locating the origin (schematic)

There is a simple rule for finding the origin: as a crack grows it keeps branching, and branches always point "away" from the origin. So trace back against the direction of branching; the point where the cracks converge is the origin.

The amount of branching also tells us how much energy the glass stored when it broke. Heat-strengthened glass or low-stress failures branch little and leave large fragments, so the origin is relatively easy to find; fully tempered glass stores a lot of energy and shatters into many small pieces, so the origin area must be pieced together carefully. In glass laminated into a module, most fragments stay stuck to the encapsulant and preserve the full crack pattern, which actually makes analysis easier.

Once the origin is found, examine the fracture surface at the origin under a magnifier or microscope: there is usually a smooth "mirror" zone at the origin, giving way outwards to a misty zone and then a rough hackle zone. In fracture mechanics, the mirror radius is related to the stress at fracture: the higher the stress, the smaller the mirror (fracture stress is roughly inversely proportional to the square root of the mirror radius). This is the classic way of estimating fracture stress in fractography.

Summary

Trace back against the branching to find the origin, then use its location to classify: an internal origin usually means spontaneous breakage; a surface impact point, impact; a crack starting at right angles to the edge, thermal stress; and origins near clamps and supports, load and installation.

04A practical workflow for analysing breakage ​

Putting these methods together gives a workflow that can be applied in practice:

Figure 3. General workflow for analysing PV glass breakage

Figure 3. General workflow for analysing PV glass breakage

  • Field record: record the location and share of broken modules, when breakage occurred and the weather; photograph the whole module and the origin area; record racking type, clamp positions and torque.
  • Locate the origin: trace back against the branching on the whole crack pattern, mark the origin, and check whether origins across several modules follow a pattern.
  • Classify: combine the origin location (internal, surface, edge) with the fragment pattern to make an initial call: spontaneous, impact, thermal stress, or load and installation.
  • Lab verification: examine the origin area under the microscope and, if needed, use SEM and EDS to confirm inclusion composition; measure surface stress and edge quality on unbroken glass from the same batch.
  • Reproduce and assign the cause: reproduce the failure through simulated load, hot-spot and similar tests, confirm the main cause, and propose improvements on the glass, module design or installation side.

As article 07 explained, field breakage usually results from several factors combined, so take particular care when assigning the cause: "origin at the clamp" shows that installation was the trigger, but not that the glass itself is blameless. Low surface stress or edge defects can equally make glass break under loads it should have withstood.

05Optical and surface failures ​

These failures do not break the glass, but they often lead to cosmetic complaints and disputes over energy yield. The key is first to tell whether the problem lies in the coating or in the glass itself.

FailureAppearanceMain causesHow to tell
Whitened / peeling coatingLocal whitening, coating flaking offPoor coating adhesion or durability; alkaline cleaners, sand abrasionCompare coated and uncoated sides; measure transmittance change
Glass weathering / white stainsHazy white stains that cannot be wiped offMoisture during storage and transport; surface alkali leaches and attacks the surfaceMostly between adjacent sheets in a pack; linked to storage conditions
Quench marks (anisotropy)Patterns visible in polarised lightUneven quenching, uneven stressObserve with a polariser; pattern matches the nozzle layout
IridescenceColoured interference fringes on the surfaceUneven coating thickness or local contaminationChanges with viewing angle; usually linked to coating process
Coating colour variationColour differs across a sheet or between batchesFluctuation in roll-coating thicknessVisual check in a standard light box plus transmittance testing

Table 2. Diagnosing optical and surface failures

Glass weathering deserves the most attention. It usually occurs in storage and transport between shipment and lamination: in damp conditions, sodium ions leach from the glass surface and form an alkaline liquid film with moisture, which in turn attacks the surface. Once weathering has formed it is essentially irreversible, lowering transmittance and impairing adhesion to the encapsulant. Controlling storage humidity, standardising packaging and using first-in, first-out are therefore the most effective preventive measures.

06Final thoughts ​

The core of glass failure analysis is to turn the outcome "the glass broke" back into a clear chain of evidence: where the origin is, what pattern the fragments show, how glass from the same batch performs, what the field conditions were, and whether the failure can be reproduced.

This chain of evidence is also the basis for assigning responsibility between material suppliers, module makers and plant owners. Many disputes cannot be settled precisely because the first steps, field recording and origin location, were not done properly.

Bottom line

Glass "talks": find the origin first, then read the pattern, and finally use testing and reproduction to turn inference into evidence.

In the next article we return to design: 3.2 mm glass-backsheet, 2.0 + 2.0 mm glass-glass, 1.6 mm thin glass—how should module glass be chosen for different applications, and how should glass thickness be coordinated with frames and racking? Stay tuned. We would be glad to hear from you.

Calculation notes / data basis: 1. The roughly 2.5–4% volume expansion when nickel sulphide transforms from the alpha to the beta phase, and the heat-soak temperature of about 260–290 °C, are from an IIBEC technical article on NiS breakage in building glazing; the relationship between mirror radius and fracture stress (σ·√r ≈ constant) follows the ASTM C1678 fracture mirror method. 2. The fracture pattern figure is schematic; actual patterns depend on glass stress level, lamination and load mode, and diagnosis should draw on several kinds of evidence. 3. The analysis workflow is a general method and can be adapted to site conditions and testing resources.

References

  1. ASTM C1678, Standard Practice for Fractographic Analysis of Fracture Mirror Sizes in Ceramics and Glasses
  2. IIBEC: Glass Breakage Analysis: The Impact of Nickel Sulfide Inclusions in Building Glazing, Part One, https://iibec.org/publication-post/glass-breakage-analysis-the-impact-of-nickel-sulfide-inclusions-in-building-glazing-part-one-understanding-and-identifying-nis/
  3. GB 15763.2—2005 Safety glazing materials in building — Part 2: Tempered glass
  4. China Photovoltaic Industry Association: T/CPIA 0028.1—2024 Glass for photovoltaic modules — Part 1: Front plate anti-reflective coated glass, 2024
  5. pv magazine: CEA recommendations for mitigating glass breakage, 2025-07-28
  6. PV Tech: NREL says thinner, taller solar modules contributing to increased rate of breakages, 2024-12-11
PV Materials Lab
https://pvmaterialslab.com
PV Materials Lab
A PV R&D and technical team with 10+ years of experience | In-depth technical knowledge sharing
Materials · Reliability · Failure Analysis · Standards & Certification · Products · Processes
Exploring AI + PV — collaboration welcome

Disclaimer:
1. Original content reflects the authors' personal views only, is for reference, and does not constitute investment advice.
2. Reposted and cited content is credited to its source, with respect for original work.
3. Some content is AI-assisted (chart generation, data retrieval, concept explanations, etc.); the core framework and key content are written by our technical team and reviewed by humans.
4. For any inaccuracy or infringement, please leave a message or contact us.